14c28n3.png

Austenitizing

Belt furnace. Time in furnace according to the table.

Thickness Thickness Time
mm in. minutes
2.5 0.100 5
3.0 0.118 6
3.25 0.128 7
3.5 0.138 8
3.75 0.148 10
4.0 0.157 12
4.9 0.192 25

Quenching

Quench as rapidly as possible. For optimal results 600°C (1110°F) should be reached within 2 minutes or less.

Deep freezing

The material only needs to reach the desired deep freezing temperature, no soaking-time is required.

Tempering , 2 hours
Hardness Temperature
62 HRC 175oC (345oF)
59 HRC 225oC (435oF)
57 HRC 350oC (660oF)